MP35N® alloy provides a combination of strength, good biocompatibility, and corrosion resistance.
Chemical composition
Composition |
ASTM F562 |
Carbon | 0.025 max |
Manganese | 0.15 max |
Silicon | 0.15 max |
Phosphorus | 0.015 max |
Sulfur | 0.010 max |
Chromium | 19.0 - 21.0 |
Nickel | 33.0 - 37.0 |
Molybdenum | 9.0 - 10.5 |
Iron | 1.0 max |
Titanium | 1.0 max |
Boron | 0.015 max |
Cobalt | Balance |
Physical properties
Metric | English | |
Density | 8.41 g/cm³ | 0.304 lbs/in³ |
Modulus of elasticity | 233 Gpa | 33.8 Mpsi |
Electrical resistivity | 1033 µohm*mm | 40.7 µohm*in |
Thermal conductivity | 11.2 W/(m*°C) | 78 BTU*in/(hr*ft²*°F) |
Coefficient of thermal expansion | 12.8 µm/(m*°C) | 7.1 µin/(in*°F) |
*Values calculated at 22 °C [72 °F]
Mechanical properties
Cold worked % |
Yield strength |
Ultimate tensile strength |
Elongation % |
0 | 855 MPa [124 ksi] | 1269 MPa [184 ksi] | 37.4 |
20 | 1282 MPa [186 ksi] | 1613 MPa [234 ksi] | 5.9 |
37 | 1620 MPa [260 ksi] | 1910 MPa [277 ksi] | 4.3 |
50 |
1793 MPa [260 ksi] | 2055MPa [298 ksi] | 3.7 |
60 |
1793 MPa [260 ksi] | 2151 MPa [312 ksi] | 3.5 |
68 |
1800 Mpa [261 ksi] | 2206 MPa [320 ksi] | 2.6 |
75 |
1868 Mpa [271 ksi] | 2261 MPa [328 ksi] | 2.5 |
80 |
1931 MPa [280 ksi] | 2310 MPa [335 ksi] | 2.3 |
84 |
1972 MPa [286 ksi] | 2344 MPa [340 ksi] | 2.8 |
87 |
2020 MPa [293 ksi] | 2372 MPa [344 ksi] | 2.5 |
90 |
2261 MPa [328 ksi] | 2551 MPa [370 ksi] | 2.0 |