302 stainless steel

302 stainless steel has increased carbon content for higher tensile strength. This material is produced using an electric-arc melt process, resulting in a high-quality austenitic stainless steel.

 

Chemical composition

Composition

ASTM A313
%

Carbon 0.12 max
Manganese 2.00 max
Phosphorus 0.045 max
Sulfur 0.030 max
Silicon 1.00 max
Chromium 17.0 - 19.0
Nickel 8.0 - 10.0
Nitrogen 0.10 max
Iron Balance

*Localized variations in final melt chemistry can cause slight changes in ultimate tensile strength when 302 stainless steel is drawn to fine wire.

 

Physical properties

  Metric

English

Density

7.89 g/cm³ 0.285 lbs/in³

Modulus of elasticity

193 GPa 28 Mpsi

Electrical resistivity

720 µohms*mm 28.3 µohms*in

Thermal conductivity

16.3
W/(m*°C)
113
BTU*in/(hr*ft²*°F)

Coefficient of thermal expansion

18.72
µm/(m*°C)
10.4
µin/(in*°F)

*Values calculated at 22 °C [72 °F]

 

Mechanical properties

Cold worked %

Yield strength

Ultimate tensile
strength

Elongation
%
0 338 MPa [49 ksi] 731 MPa [106 ksi] 48
20 862 MPa [125 ksi] 1014 MPa [147 ksi] 9.8
37 1165 MPa [169 ksi] 1303 MPa [189 ksi] 3.2
50 1351 MPa [196 ksi] 1517 MPa [220 ksi] 2.6
60 1531 MPa [222 ksi] 1682 MPa [244 ksi] 2.2
68 1675 MPa [243 ksi] 1882 MPa [273 ksi] 2.1
75 1731 MPa [251 ksi] 1993 MPa [289 ksi] 2.4
80 1944 MPa [282 ksi] 2130 MPa [309 ksi] 2.2
84 2034 MPa [295 ksi] 2255 MPa [327 ksi] 2.2
87 2068 MPa [300 ksi] 2289 MPa [332 ksi] 2.3
90 2199 MPa [319 ksi] 2379 MPa [345 ksi] 2.2
92 2220 MPa [322 ksi] 2558 MPa [371 ksi] 2.5

*All data represent results from 25.4 cm [10 in] test gauge length.
Values are typical and may not represent all diameters. Test method will affect results.

302 stainless steel

302 stainless steel has increased carbon content for higher tensile strength. This material is produced using an electric-arc melt process, resulting in a high-quality austenitic stainless steel.

 

Chemical composition

Composition

ASTM A313
%

Carbon 0.12 max
Manganese 2.00 max
Phosphorus 0.045 max
Sulfur 0.030 max
Silicon 1.00 max
Chromium 17.0 - 19.0
Nickel 8.0 - 10.0
Nitrogen 0.10 max
Iron Balance

*Localized variations in final melt chemistry can cause slight changes in ultimate tensile strength when 302 stainless steel is drawn to fine wire.

 

Physical properties

  Metric

English

Density

7.89 g/cm³ 0.285 lbs/in³

Modulus of elasticity

193 GPa 28 Mpsi

Electrical resistivity

720 µohms*mm 28.3 µohms*in

Thermal conductivity

16.3
W/(m*°C)
113
BTU*in/(hr*ft²*°F)

Coefficient of thermal expansion

18.72
µm/(m*°C)
10.4
µin/(in*°F)

*Values calculated at 22 °C [72 °F]

 

Mechanical properties

Cold worked %

Yield strength

Ultimate tensile
strength

Elongation
%
0 338 MPa [49 ksi] 731 MPa [106 ksi] 48
20 862 MPa [125 ksi] 1014 MPa [147 ksi] 9.8
37 1165 MPa [169 ksi] 1303 MPa [189 ksi] 3.2
50 1351 MPa [196 ksi] 1517 MPa [220 ksi] 2.6
60 1531 MPa [222 ksi] 1682 MPa [244 ksi] 2.2
68 1675 MPa [243 ksi] 1882 MPa [273 ksi] 2.1
75 1731 MPa [251 ksi] 1993 MPa [289 ksi] 2.4
80 1944 MPa [282 ksi] 2130 MPa [309 ksi] 2.2
84 2034 MPa [295 ksi] 2255 MPa [327 ksi] 2.2
87 2068 MPa [300 ksi] 2289 MPa [332 ksi] 2.3
90 2199 MPa [319 ksi] 2379 MPa [345 ksi] 2.2
92 2220 MPa [322 ksi] 2558 MPa [371 ksi] 2.5

*All data represent results from 25.4 cm [10 in] test gauge length.
Values are typical and may not represent all diameters. Test method will affect results.